Before I lay down the glass, I have found that I can create a better bond with my corecell foam if I first give the foam a skim coat of epoxy / microballoons / aerosil .
Here's my recipe for my skim coat :
300ml B side
600ml A side.........mix with drill mixer
then mix in the dry stuff :
* 2000ml aerocil ( fumed silica;wicked stuff don't breath it)
* 1000ml glass microballoons
It ends up being like fluffy white cake frosting and the aerosil keeps it from running.
2.16.2008
skim coat the foam before laying down the glass
Subscribe to: